Written by the crimp and assembly engineering team at OBD-Cable. 21 years of terminal crimping, cross-section work and diagnostic harness assembly for test-bench builders and OEM programmes.
There is a returns bin in every harness shop. In ours it held 11 J1962 cables that had measured between 0.3 and 0.5 mΩ on the day they shipped, and between 3 and 6 mΩ when they came back 18 months later. Every one of them had a crimp height inside the drawing window. Every one of them had passed a pull test.
That bin is why this article exists.
The short answer, before the argument
Compression ratio describes what the crimp did to the metal. Crimp height is the number you can actually hold on a production line. Contact resistance is neither of those — it is the contact pressure that survives thermal cycling, and that pressure is set by the compression ratio your process lands on, not by the height somebody wrote on the setup sheet.
So the ordering that survives an audit is this: compression ratio is the physics, crimp height is the handle, and a crimp height window is worth nothing until a polished cross-section proves it lands inside a compression-ratio band.
If the question forces a single answer: compression ratio controls contact resistance. Crimp height predicts it. Neither one is the mechanism. The mechanism is the contact pressure that is still there after 500 thermal cycles.
If you copied a crimp height from a terminal datasheet, set the press to it, passed a pull test, and shipped, you are controlling a number that correlated with quality on a different wire, a different terminal lot, and a different applicator. It works until one of those three changes. Then it fails quietly, which is the worst way for anything to fail.
Two numbers, and the one that lies to your control plan
Ask any crimp standard to define crimp height and you get the same sentence back: barrel height after the tool closes, measured with a blade anvil across the flat at the middle of the conductor crimp. Correct, and useless on its own. The number only repeats if the anvil lands in the same place every time, and in most shops nobody ever wrote down where that place is. Put it over the seam and it reads high, because the seam never fully closes. Put it over the front bellmouth and it reads low, because the bellmouth flares. Both readings look reasonable on a form. Both are wrong, and both become somebody’s reject rate six months later.
Compression ratio is copper-in versus space-out:
CR = (A_wire ÷ A_crimp) × 100%
A_wire is what the copper actually measures — strand count times strand area, from the construction on the drawing, never the nominal figure printed on the reel. A_crimp is the internal cross-sectional area of the conductor barrel, taken on a polished cross-section at the centreline. Void fraction is one minus CR, so a 78% ratio is a 22% void fraction.
Two things to settle before you argue with anyone about this.
Some drawings invert the formula and call the inverse “compression ratio.” A 125% reading on their sheet is our 80%. Ask which way the number runs before you decide whether a part is in spec. We have watched two hours of a customer meeting evaporate over this exact confusion.
And use the real strand sum. The label is a nominal number, and nominal numbers drift:
| Nominal size | Construction | Actual copper area | How it behaves at the press |
| 0.35 mm² | 7 × 0.25 mm | 0.344 mm² | Coarse, stiff, forgiving |
| 0.35 mm² | 12 × 0.19 mm | 0.340 mm² | Standard signal cavity wire |
| 0.50 mm² | 19 × 0.18 mm | 0.484 mm² | Most common in J1962 cavities |
| 0.50 mm² | 37 × 0.13 mm | 0.491 mm² | Finer, better flex life, wants its own pull curve |
| 0.50 mm² | 105 × 0.08 mm | 0.528 mm² | High-flex, ISO 6722 class, easy to damage |
| 1.00 mm² | 19 × 0.26 mm | 1.009 mm² | Power and ground pins |
Look at the three 0.50 mm² rows. Three reels, same label, 9% apart in actual copper. Run all three at the same crimp height and you get three different compression ratios, three different pull forces, and one of them sits outside the acceptable void band without anyone noticing, because the label agreed.
That is the first way this problem gets in. There are three more.
Where it goes wrong: four scenes from a shop floor
Purchasing finds a second source. A reel gets swapped. Same nominal size, same colour, same supplier code on the box. Crimp height stays at 1.15 mm because nobody thinks to change it, and why would they — the label says 0.50 mm². Pull test still passes comfortably. Six weeks later a customer reports intermittent CAN dropouts on one batch. The cross-section shows 92% compression and two fractured strands at the rear bellmouth. Nothing in the paperwork was violated. Nothing in the paperwork would have caught it either.
The applicator wears in. An anvil runs 380,000 cycles. The indenter tip loses 0.04 mm. Effective crimp height drifts from 1.15 to 1.19 mm across about 3 weeks. Pull force falls 22% but stays above the 60 N drawing minimum, so every lot is accepted. Compression ratio is now 69%. Contact resistance climbs from 0.9 to 3.4 mΩ. The only instrument that saw it coming was an SPC chart on crimp height, and only because somebody was actually plotting it instead of filing it.
An operator measures with a caliper. The blade micrometer went to the calibration lab on Friday. The caliper reads 0.04 mm high, because its flat anvils bridge the flash at the seam and the burr at the formed edges. The operator adjusts the press down to compensate, because the reading says the crimp is too tall and the reading is trusted. Real crimp height is now 1.11 mm, compression ratio is 87%, and the entire shift is over-crimped. This is the most common measurement error we find in incoming audits, and it always looks like diligence.
A drawing is copied from a different terminal family. A customer sends a 1.15 mm crimp height for a 0.64 mm terminal. The number came from an older drawing for a 0.50 mm series terminal with a thicker barrel wall. Same number, different metal volume, 11 points of compression ratio apart. First article passes, because first article was crimped on the customer’s sample tooling, which was set up years earlier by somebody who did the cross-sections properly and then retired.
In all four scenes the crimp height was in spec and the contact resistance was not. That is the whole failure, in one line.
What is actually holding the joint together
Current does not use the area you can see. It crowds into microscopic asperity spots where the two surfaces genuinely touch, and the resistance of those spots is constriction resistance. For a single equivalent contact spot, Holm’s result gives resistance falling as one over the square root of contact force. Double the force, and constriction resistance drops about 30%. That relationship is a simplification — real interfaces are a distribution of spots, not one — but the direction and the order of magnitude hold, and nothing else in the crimp changes them.
Riding on top of the constriction term is film resistance. Tin-plated brass carries a thin oxide that regrows. Copper carries its own. A good crimp breaks that film through bulk deformation and creates fresh metal-to-metal contact, part of it cold-welded, and that welded fraction is what carries current for the next decade. A poor crimp leaves the film intact and lets the joint ride on asperity contact alone. That is survivable until vibration and thermal expansion work the interface loose.
Most training material skips the next part, and it is the part that decides whether your cable comes back. A crimp is a spring. The barrel is formed, yielded, and allowed to spring back against the wire bundle. What holds the interface together for the life of the part is not the force of the press — the press is long gone. It is the residual elastic stress locked into the formed barrel. That residual stress is the entire pressure budget, and it is finite.
This is not a new observation. Patent literature describes it precisely: cold welding and residual force distribution are two independent mechanisms that both have to hold, and the barrel maintains contact because the conductor and the barrel recover elastically by different amounts. TE’s own white paper on crimp height makes the related argument that height plus crimp force beats destructive sampling for process control. A 2024 paper in the IOP Conference Series ran 45 crimped assemblies through thermal shock under SAE/USCAR-21 and EN 60352-2 protocols and found a statistically significant relationship between crimp height and resistivity before and after. That work is useful confirmation. It is also the reason we stopped treating “in spec at receiving” as the finish line.
Brass does not keep a spring forever. At 125 °C it lets go faster, and 125 °C is where a surprising share of our product spends its worst hours. Tin oxide regrows wherever the interface is no longer gas-tight. Contact pressure decays, resistance climbs, temperature climbs, relaxation accelerates. It is a loop, and it runs on a timescale of months, which is exactly the timescale that hides it from every test you run on the shipping dock.
So the failure mode that matters is not “the crimp was loose at incoming inspection.” It is “the crimp had plenty of residual stress at incoming inspection and spent it.”
Why crimp height alone cannot carry this
Crimp height is a one-dimensional proxy for a two-dimensional area. It is fast. It is non-destructive. It repeats to a thousandth of a millimetre. And it is completely blind to how that area was achieved. Two crimps at 1.42 mm can be 15 points of compression ratio apart if the barrel wall thickness or the terminal temper differs between lots. Height tells you the die closed to a number. It does not tell you what happened to the metal underneath it.
Compression ratio is the measurement that actually describes the crimp. It is also the one you cannot sample. You have to destroy the part, mount it in epoxy, grind to the centreline, polish to one micron, and measure area under a microscope — twenty minutes per part with someone who knows what they are looking at. So it lives in qualification and audit, and crimp height lives on the line. It is operator-sensitive in the other direction too: a coarse grind smears copper across the voids, and a 22% void fraction suddenly photographs as 4% and everybody goes home pleased.
There is a third problem, and it catches experienced people. Compression ratio and pull strength can move in opposite directions. Two crimps at identical compression ratio can pull at very different forces, because pull force also depends on strand damage at the bellmouth, seam closure, and where the fracture initiates. Qualify on ratio alone and you can approve a joint that carries current beautifully and snaps at 30 N.
Most arguments about terminal crimp quality are really arguments about which of those two numbers somebody wrote on the control plan. You need all four measurements, taken at different points in the process lifecycle. Skipping one does not simplify the job. It moves the discovery to a worse place.
The case: a cable that passed everything and still came back
A European test-bench integrator sent us 16-pin J1962 assemblies, 1 m, moulded overmould, 0.50 mm² 19-strand on the signal cavities and 1.00 mm² 19-strand on power and ground. Pins 4, 5 and 16 carry the supply to a pass-through device, and in their application those pins sit near 8 A for hours at a time inside a sealed shell.
The cable passed continuity. It passed hipot. It passed pull test at first article, and it passed the customer’s own receiving inspection. It failed after 500 thermal cycles between -40 and +125 °C, with 30-minute dwells. Contact resistance on the ground pin had climbed from 0.36 to 3.9 mΩ. Two units out of 30 opened completely during the vibration run that followed.
We cut the parts. Compression ratio on the 1.00 mm² pins was 87%. Barrel wall at the thinnest point was 0.203 mm against a nominal 0.235 mm — 14% thinning. Seam closed, with a visible notch. Pull force was 172 N, which is excellent, which is precisely why nobody had looked harder.
The press had been left at 1.37 mm instead of the 1.42 mm nominal. Not by accident. After a tooling change two years earlier, somebody had run a pull test at the bottom of the window, seen a number 3% higher, and decided the low end was “the better setting.” Nobody ever cross-sectioned a part to check what that 3% was buying.
The number worth sitting with is this one. At 1.37 mm the initial contact resistance was better than nominal — 0.36 mΩ against 0.48. The over-crimped parts were outperforming the correct parts on the only electrical test anybody was running, and they pulled harder. Every indicator on the shipping dock said these were the best cables on the line.
Then the pressure relaxed. After the thermal run the 1.37 mm parts sat at roughly 98 MPa and 3.9 mΩ. The nominal parts sat at 142 MPa and 0.62 mΩ.
One more measurement decided the diagnosis. A pressure drop from about 205 to 98 MPa should raise constriction resistance by roughly 45%, using the square-root relationship. We measured a factor of nearly 11. The rest of that rise was not mechanical. It was oxide regrowth at an interface that had lost its gas-tight seal and its cold-welded fraction. A relaxed crimp does not fail because it is loose. It fails because it stops being sealed, and the film returns.
The thermal loop then does the rest. At 8 A, 3.9 mΩ burns 0.25 W in a joint that should be burning 32 mW. Inside a sealed connector shell that is a measurable temperature rise, and the temperature rise accelerates the stress relaxation that produced the resistance. Slow, stable, and invisible to any test shorter than a month.
We rebuilt the window from cross-sections on that exact wire and terminal combination, moved nominal back to 1.42 mm, and made a cross-section mandatory at every setup and every terminal lot change. Drift on the rebuilt assemblies over 500 cycles was 0.14 mΩ.
The window, mapped
This is the table we build for every new wire and terminal combination before a single production part is crimped. It is 1.00 mm² 19-strand into a 1.0 mm series terminal, tin-plated brass barrel, measured four-wire Kelvin at 20 mV open circuit and 100 mA maximum, at 20 ± 2 °C after 24 hours of stabilisation. Our drawing calls for 110 N minimum pull.
| Crimp height | Compression ratio | Initial R | R after 500 cycles | Thinnest wall | Pull force | Verdict |
| 1.32 mm | 92% | 0.32 mΩ | 5.4 mΩ | 0.196 mm | 165 N | Over-crimp. Best numbers at receiving, worst numbers in year two. |
| 1.37 mm | 87% | 0.36 mΩ | 3.9 mΩ | 0.203 mm | 172 N | Top edge. Where the case-study press was sitting. |
| 1.42 mm | 80% | 0.48 mΩ | 0.62 mΩ | 0.234 mm | 171 N | Nominal. This is what we ship. |
| 1.47 mm | 73% | 0.79 mΩ | 1.1 mΩ | 0.238 mm | 158 N | Bottom edge. Survivable, not comfortable. |
| 1.52 mm | 66% | 2.2 mΩ | 4.6 mΩ | 0.240 mm | 118 N | Under-crimp. Loose strands, moisture path, fails pull on finer wire. |
Two things jump out, and neither is visible on a datasheet.
The first is sensitivity. Between 1.37 and 1.47 mm — 0.1 mm, about the thickness of a sheet of copy paper — compression ratio moves 14 points. On this terminal and wire, 50 µm of height is worth roughly 7 points of ratio. That is why “plus or minus 0.05 mm” is not a comfortable tolerance. It is the entire useful range of the process, halved.
The second is the shape of the pull curve. It peaks around 1.37 to 1.42 and falls away on both sides. On the tight side it is a terrible discriminator: 165 N at 92% compression clears a 110 N minimum by 50%. If pull force is your only acceptance criterion, you own a test that catches under-crimp reliably and waves over-crimp straight through to the customer. Over-crimp is the failure mode that reaches the field.
The rules of thumb we actually use
None of these replace a cross-section. They are the numbers that tell you whether to stop the press and cut a part.
- Compression ratio 75 to 85%: good. This is where we aim.
- Above 88%: reject. Over-crimp, wall thinning, stress relaxation waiting to happen.
- Below 70%: reject. Under-crimp, loose strands, moisture ingress path.
- Wall thinning above 15% of nominal: reject regardless of what the ratio says.
- Bellmouth 0.2 to 0.5 mm at the rear: outside that, you have a stress riser or you have lost contact area.
- Seam closed with no through-wall gap. An open seam is a wick, not a crimp.
- No fractured strands at the bellmouth. One fractured strand out of 19 removes about 5% of the copper from that section and most of the fatigue life with it.
Setting a window that holds: the procedure
This is the sequence we run to build a crimp height window on every new terminal and wire pair. It takes 2 days, and it is the only route we have found to a window that is an engineering decision rather than a copied number.
- Freeze the inputs and write them down. Exact wire construction including strand count and diameter, terminal part number and revision, plating type and thickness, barrel wall thickness measured on the incoming lot, applicator model, press, shut height. Every one of those variables moves the answer. Nothing changes during qualification, and the written record is what you pull out in two years when somebody asks why the window is what it is.
- Take the supplier’s bracket as a bracket. The terminal maker will give you a crimp height range for a wire size class. Treat it as a starting point and a sanity check. It is not a specification for your wire, and it was not derived on your applicator.
- Run the pull-force curve first. 10 heights across and slightly beyond the bracket, 10 samples each, 25 mm per minute. Plot pull force against height. You are looking for the plateau, not the peak. The peak is a fragile operating point. The plateau is where a process can live for a decade.
- Cross-section at 5 heights, 3 stations each. Mount, grind to the centreline, polish to one micron, do not etch. Measure compression ratio at front, middle and rear of the conductor crimp. Measure wall thickness at the thinnest point top and bottom. Check seam closure, bellmouth length at both ends, and count fractured or nicked strands. Photograph every one at the same magnification so this year’s section can sit beside last year’s without an argument.
- Apply hard rejection limits before you look at the electrical data. We reject any height above 88% compression, above 15% wall thinning, with an open seam, with a bellmouth under 0.2 mm or over 0.5 mm, or with any fractured strand. Setting limits after you have seen the resistance results is how a team talks itself into a bad window and then defends it for three years.
- Measure resistance, then thermal-cycle the best three. Four-wire Kelvin, 20 mV open circuit, 100 mA maximum, 24 hours of stabilisation at 20 °C. Then 500 cycles between -40 and +125 with 30-minute dwells, re-measuring after each run. This step is what separates a window that passes receiving from a window that survives a vehicle.
- Set the window to the intersection, then trim to the middle 60%. Take the overlap of the pull plateau, the compression band, the wall-thickness limit and the drift limit. Then do not use the whole overlap. Use the middle 60% of it. The edges of a valid range are valid on the day you measured them and stop being valid the first time a terminal lot runs 0.02 mm tall.
- Lock it down. Control plan entry, SPC limits at one third of the window, gauge calibration schedule, and a written re-qualification trigger list. Without the trigger list, the window quietly expires and nobody notices for a year.
Our trigger list is deliberately blunt: any change of wire supplier or construction; any terminal lot whose incoming barrel height differs by more than 0.02 mm; any applicator rebuild, tip change or crash; any press change; and any SPC trend of 0.02 mm in the same direction across 3 consecutive samples. That last line has caught two tooling failures before they produced a single reject.
How to measure crimp height without introducing a 0.04 mm error
Four measurements answer four different questions. Using one to answer another is where a quality system develops its blind spots.
| Method | Question it answers | Destructive | Frequency | Practical resolution |
| Blade-anvil crimp height gauge | Did the die close to the setpoint? | No | Every setup, then SPC every 2 hours or 5,000 crimps | 0.001 mm |
| Digital caliper | Roughly how tall is the part? | No | Never for acceptance | 0.01 to 0.02 mm, biased high |
| Metallographic cross-section | What did the crimp do to the metal? | Yes | Every setup, every terminal lot change, once per shift on running work | Area measurement plus visual |
| Four-wire Kelvin resistance | Is the interface electrically sound right now? | No | Qualification plus lot audit | 0.01 mΩ |
| Pull test | Will it hold mechanically? | Yes | Every lot, per wire size | 1 N |
| Thermal cycling with R monitoring | Will it still be sound in year eight? | Time, not parts | Qualification and annual re-validation | 0.01 mΩ per channel |
Two notes on the two that people get wrong most often.
A caliper measures the highest points on the part. On a crimped barrel, the highest points are the flash at the seam and the burr at the formed edges, so the bias is systematic: typically 0.03 to 0.05 mm high, which on the wire in our table is 5 to 8 points of compression ratio. It is not a small error and it does not average out, because it always leans the same way. A blade anvil spans the barrel and reads formed height. If your micrometer is at the calibration lab, stop the press. Do not substitute.
Cross-section preparation quality decides the answer, which is why crimp cross-section analysis is worth paying a metallographer for rather than a technician with a saw. A saw cut smears copper across the voids and a coarse grind does the same thing more subtly. You want a polished surface where voids read as clean black shapes with sharp edges. If the voids look grey or fuzzy, you are looking at your own polishing compound, not at the crimp. Cut at the centreline of the conductor crimp, and if the section is not symmetric front to back, you missed the centreline and your area measurement is fiction.
What the section has to show:
| Feature | Target | Why it matters |
| Conductor compaction | 80–90% of nominal cross-section | Below 80%, strands move under vibration |
| Void fraction | Under 10% | Voids are where corrosion starts |
| Bell-mouth | 0.2–0.5 mm | Too little causes strand cut-off; too much reduces retention |
| Cut-off burr | Under 0.1 mm | Burrs act as stress risers and can pierce insulation |
| Heel/toe cracks | None visible | A crack at the heel is a fatigue origin, not a cosmetic defect |
Symptoms, and what they usually mean
Most incoming questions arrive as a symptom, not a measurement. This is the mapping we use to decide where to cut first.
| Passes pull test, fails thermal cycling | Over-crimp and stress relaxation | Cross-section wall thickness and compression ratio at the thinnest point |
| One lot fails pull, next lot is fine | Tool wear drifting or a tall terminal lot | Crimp height trend over the last 20 samples, plus incoming barrel height on the suspect lot |
| Resistance fine cold, climbs when warm | Differential expansion plus film regrowth | Resistance measured at temperature, not after cool-down |
| Intermittent opens under vibration | Strand fracture at the rear bellmouth | Section the bellmouth, count fractured strands, check bellmouth length |
| Green residue or corrosion at the crimp | Moisture ingress through an open seam or a cut insulation crimp | Seam closure on the cross-section, insulation crimp grip by axial pull |
| Random high resistance on 1 part in 500 | Mis-fed terminal or a damaged applicator tip | Section three rejects, look for asymmetric barrel forming |
Five mistakes we keep seeing
- Copying a crimp height from a datasheet or a customer drawing and calling it a process. That number was valid for one wire, one terminal lot, one plating thickness and one applicator. Change any of them and it is a guess with a tolerance attached. Treat the datasheet as a bracket, not an answer.
- Treating pull force as the acceptance criterion. Pull force catches under-crimp reliably and over-crimp almost not at all. The over-crimped part in our case study pulled at 172 N against a 110 N minimum. It was the strongest cable in the batch and the only one that failed in the chamber.
- Measuring resistance with a two-wire multimeter. At the milliohm level, lead resistance and probe contact resistance are larger than the thing you are trying to measure. A two-wire reading of “0.02 ohms, looks fine” tells you nothing except that the circuit is not open. You need four-wire Kelvin, low test current and a stable temperature. Anything else is theatre.
- Ignoring the insulation crimp. The conductor crimp carries current. The insulation crimp carries mechanical load and keeps moisture out of the strand bundle. An insulation crimp that pierces the insulation creates a stress riser and a corrosion site at the same point, and it will not show up in any electrical test. Check it by axial pull and visual deformation, not by height.
- Never re-qualifying. The window was correct in March. By November the wire supplier changed a stranding line, the terminal lot runs 0.02 mm taller, and the applicator has 300,000 cycles on it. The window is now wrong and every document still says it is right. This is where “but we have always done it this way” comes from, and it is the most expensive sentence in manufacturing.
How to know the fix is real
A fix is confirmed when four independent measurements agree. Not when the line starts running again.
- Capability on crimp height. 30 consecutive pieces, measured with the blade micrometer at the specified location. You want Cpk of at least 1.33 against the window, and you want the mean near the centre rather than hugging a limit. A mean of 1.40 on a 1.37 to 1.47 window has not fixed anything. It has moved the risk.
- Cross-section agreement. 3 parts from the run, 3 stations each, compression ratio inside the band at all 9 measurement points. Not on average — at every point. A crimp that measures 80% in the middle and 90% at the front is a crimp with a taper, and the taper is where the fracture starts.
- Resistance, before and after. Four-wire Kelvin at the specified test current, 500 thermal cycles, measured again. The number that matters is the drift, not the absolute value. A joint that starts at 1.2 mΩ and stays within 0.3 is a better joint than one that starts at 0.4 and climbs to 4.
- Pull force on the same parts you sectioned. If the parts that cross-sectioned cleanly also pull at the top of the plateau, the window is doing what you think it is doing. If they do not, one of your two measurements is lying and you need to find out which before you ship anything.
Only when those four agree do we sign the window off and release it to the control plan.
How we hold the window on the line
Setting a window takes an afternoon of metallography. The hard part is the 21 years after it.
Crimp height runs on SPC at every press, sampled every 2 hours or every 5,000 crimps, with limits at one third of the drawing window. Blade micrometers sit on a 90-day calibration cycle against gauge blocks, and no press runs without one on the bench. Cross-sections are cut at every setup, every terminal lot change, and once per shift on running work, photographed at fixed magnification so this month’s section can be laid next to last year’s without a discussion.
Incoming material gets its own gate. Barrel height, plating thickness and temper are checked on every terminal lot, because a lot that runs 0.02 mm tall silently shifts every crimp on the line. Wire is checked for actual strand count and strand diameter against the drawing construction, not against the reel label — the table earlier in this article is exactly why.
What we actually send with the parts
We supply PPAP at Level 3. The element customers actually read is the one most suppliers leave thin: the crimp cross-section package with the height window derivation behind it. If somebody asks why nominal is 1.42 mm and not 1.37, that package answers with 9 measurement points and a thermal run, not with a datasheet. The IATF 16949 control plan is where that window lives, which is why changing it needs a signature and not an email.
The salt spray cabinet sits next to the metallography bench for a reason. A 96-hour ASTM B117 run on tin-plated terminals tells you whether the plating survives. It does not tell you whether the crimp does. So every salt spray batch also gets a four-wire resistance reading before and after, and a section cut from the same panel. We have rejected plating lots that passed the visual criteria because the resistance had drifted past 0.3 mΩ — which is the failure the customer would have hit in year two, not the rust they would have seen in week one.
We hold IATF 16949, ISO 9001 and ISO 14001, with RoHS and REACH declarations on materials and CE and UL marking where the assembly calls for it. The shop runs 5S. The warehouse is climate-controlled at 23 ± 3 °C and below 60% RH, for a boring reason: tin-plated terminals oxidise in storage, and an oxidised terminal crimps differently from a fresh one. Inspection runs in four steps — incoming, first article, in-process, final — and every assembly is electrically tested, with continuity plus hipot on the diagnostic parts whose specifications ask for it.
The last window we lost was because a blade micrometer went to calibration on a Friday and nobody stopped the press. The window was fine. The discipline around it was not.
Where this matters most: diagnostic cable
Diagnostic cable is an unforgiving place to learn crimping. The cavities are small, the wire is fine, the connector is sealed, and the consequences of a marginal joint are intermittent faults that nobody can reproduce on a bench.
The 0.64 mm terminals in most J1962 cavities are typically rated around 5 A continuous, and 1.0 mm terminals on the power and ground pins run higher. Put 8 A through a joint at 3.9 mΩ instead of 0.5 and you are dissipating 0.25 W inside a sealed shell, per pin. That heat raises terminal temperature, which accelerates the stress relaxation that produced the resistance in the first place. The loop closes on itself over months, quietly, and the first symptom is usually a U-code nobody can explain.
A marginal OBD cable crimp rarely announces itself as a crimp problem. It arrives as a bus error, a dropped frame, or a scanner that works on one vehicle and not the next. Most of the OBD cable we build exists because somebody had one of those codes and decided to design the cable out of the problem rather than replace it every quarter. OBD2 and J1962 assemblies with 0.64 and 1.0 mm terminals, moulded and assembled 16-pin connectors, CAN and CAN FD test leads, breakout boxes, extension cables, and custom diagnostic harnesses built to a customer’s pinout. We mould full-plastic connector shells rather than sourcing a metal-backshell equivalent, because the plastic body is what keeps the pin retention consistent across batches.
Gauge, length, colour, overmould profile, strain relief, branding and connector keying are all open to specification, because most of what we ship is not a catalogue part. It is somebody’s drawing with a strain relief added, a different overmould durometer, and a keying that stops it plugging into the wrong port on a bench. We quote from the drawing, not from a list.
If your drawing has a crimp height on it and no cross-section behind it, that is worth a conversation before the tooling gets cut.
Questions we get asked, answered directly
Is crimp height or compression ratio more important?
Compression ratio is the more meaningful measure of terminal crimp quality. Crimp height is the only one you can control in production. You need the ratio to prove the height is right, and the height to hold the ratio. Choosing between them is the wrong question.
What is a good compression ratio for a crimped terminal?
For automotive open-barrel crimps we work to 75 to 85%, with 70% as a floor and 88% as a ceiling before we reject. Your customer’s specification overrides this, and some European OEM specifications set the value directly rather than leaving it to the supplier.
Can I measure crimp height with a digital caliper?
You can, and it will read 0.03 to 0.05 mm high, consistently, because flat anvils bridge the seam flash and the edge burr. On a 0.50 mm² crimp that bias is worth 5 to 8 points of compression ratio. Use a blade anvil that spans the barrel.
Why did my crimp pass pull test and still fail in the field?
Because over-crimp produces the highest pull force on the curve and the worst long-term resistance. Pull force discriminates well on the loose side and poorly on the tight side. The over-crimped part in our case study pulled at 172 N against a 110 N minimum, and it was the one that failed.
Does strand count change the correct crimp height?
At a fixed height, compression ratio barely moves with strand count, because copper volume and barrel volume are both fixed. What changes is where strand damage begins and how force distributes through the bundle. Finer strand wire usually wants a slightly taller crimp and always wants its own pull curve.
What contact resistance should an OBD cable crimp have?
On a 0.50 mm² conductor into a 0.64 mm terminal we expect roughly 0.7 to 1.2 mΩ measured four-wire at 20 °C. On 1.00 mm² power pins, roughly 0.4 to 0.7. The absolute number matters less than the drift: a joint that starts at 1.0 and stays within 0.3 after 500 cycles is a good joint. One that starts at 0.4 and climbs to 4 is not.
How often should crimp height be checked on the line?
At every setup, then every 2 hours or every 5,000 crimps, whichever comes first, with SPC limits at one third of the drawing window. Immediately after any tooling change, any crash, and any terminal lot change.
What is the difference between the conductor crimp and the insulation crimp?
The conductor crimp carries current and is controlled by crimp height and compression ratio. The insulation crimp carries mechanical load and seals the strand entry, and it is set to grip without cutting through the insulation. A tight insulation crimp is a stress riser and a corrosion site, and no electrical test will find it.
What does a bad crimp actually look like on a cross-section photograph?
Voids that read as grey or fuzzy rather than clean black, a barrel wall that thins by more than 15% at one point while staying thick at another, a seam that never closed, a bellmouth that is missing at the rear, and strands flattened into a single sheet with no visible separation. Any three of those together and the crimp is out, whatever the height gauge said.
Can you crimp 105-strand high-flex wire on the same setting as 19-strand?
No. Same nominal size, roughly 9% more copper, far more initial void, and strands that damage at a much lower load. If you run it at the 19-strand height you will usually land inside the pull-force plateau and outside the strand-damage limit, which is the worst combination because both tests pass. It needs its own curve.
How do I set a crimp height window for a new terminal?
Pull-force curve across 10 heights, cross-sections at 5, compression ratio and wall thickness at 3 stations each, dry-circuit resistance, then thermal cycling on the best three. Set the window to the intersection of all four, then use only the middle 60% of it.
What documentation should a cable supplier give me?
The crimp height window with the derivation behind it, cross-section photographs at a stated magnification, pull-force data, four-wire resistance before and after environmental exposure, and material and plating certificates. If the window arrived as a number in an email with no cross-section attached, it is a guess. The twelve records worth asking for are a better starting point than a datasheet.
Talk to the people who cut the parts
If you are working through a crimp problem on a diagnostic cable — a window that will not hold, a joint that passes everything on the dock and fails in the chamber, a drawing that came from somewhere else — send it to us. We will look at the wire construction, the terminal and the application before anybody quotes anything, because most of these problems are decided before the first part is crimped.
OEM work is the majority of what we do, and the engineering support that comes with it is not a PDF: cross-section reports at magnification, PPAP packages with the window derivation included, salt spray data with resistance readings on both sides, and a straight answer about whether your window is achievable on your wire.
WhatsApp: message Linda directly — a photo of the cross-section or the drawing is enough to start. https://api.whatsapp.com/send/?phone=8617307168662&text=Need+Help%3F+Chat+linda+WhatsAPP&type=phone_number&app_absent=0
Contact page: send the details here if you would rather write it out. Wire construction, terminal part number, crimp height you are running, and the failure you are seeing. That is enough for a useful first reply. https://obd-cable.com/contact/